TableĀ 6 Tensile strength test results in grab method for finished fabric in warp and weft way

From: Efficacy of whip roller setting on physical attributes of denim fabric

Test direction Specimen no. Whip roller position Maximum force (N) Elongation at max. force (%) Force at rupture (N) Elongation at rupture (%) Time to break (s)
Warp way 1 Height 8, depth 4 620.45 34.9 411.9 35.07 0.42
2 Height 10, depth 4 620.24 29.26 450.22 29.43 0.35
3 Height 12, depth 4 626.8 34.44 489.2 34.57 0.41
4 Height 14, depth 4 688.06 35.86 497.37 35.99 0.43
5 Height 16, depth 4 592.94 32.9 459.89 33.03 0.39
6 Height 12, depth 3 612.22 37.25 439.88 37.38 0.44
7 Height 12, depth 5 564.41 33.48 424.24 33.73 0.4
Weft way 1 Height 8, depth 4 305.63 17.34 238.83 17.67 0.21
2 Height 10, depth 4 419.69 18.6 289.19 18.77 0.22
3 Height 12, depth 4 418.33 18.34 327.72 18.55 0.22
4 Height 14, depth 4 422.42 16.27 328.69 17.13 0.2
5 Height 16, depth 4 413.2 17.81 303.06 17.9 0.21
6 Height 12, depth 3 428.39 18.01 316.51 18.1 0.21
7 Height 12, depth 5 385.42 19.17 302.44 19.25 0.23